第四节 细晶粒承压钢板和承压钢管
一、ISO标准正火状态供应的细晶粒承压钢板[ISO2604/8:1985]
1.ISO标准正火状态供应的细晶粒承压钢板的钢号与化学成分,见表4-2-24
表4-2-24 正火状态供应的细晶粒承压钢板的钢号与化学成分(质量分数)(%)
| 钢号① |
C |
Si |
Mn② |
P≤ |
S≤ |
Cr≤ |
Mo≤ |
Ni≤ |
Cu≤ |
其他③ |
| P355N |
≤0.20 |
≤0.50 |
0.90-
1.60 |
0.035 |
0.035 |
0.25 |
0.10 |
0.30 |
0.35 |
N≤0.020 |
| P355NH |
≤0.20 |
≤0.50 |
0.90-
1.60 |
0.035 |
0.035 |
0.25 |
0.10 |
0.30 |
0.35 |
N≤0.020 |
| P355NL |
≤0.18 |
≤0.50 |
0.90-
1.60 |
0.030 |
0.030 |
0.25 |
0.10 |
0.30 |
0.35 |
N≤0.020 |
| P390N |
≤0.20 |
≤0.50 |
1.00-
1.60 |
0.035 |
0.035 |
0.30 |
0.30 |
0.70 |
0.50 |
N≤0.020 |
| P390NH |
≤0.20 |
≤0.50 |
1.00-
1.60 |
0.035 |
0.035 |
0.30 |
0.30 |
0.70 |
0.50 |
N≤0.020 |
| P390NL |
≤0.20 |
≤0.50 |
1.00-
1.60 |
0.030 |
0.030 |
0.30 |
0.30 |
0.70 |
0.50 |
N≤0.020 |
| P420N |
≤0.20 |
≤0.50 |
1.00-
1.70 |
0.035 |
0.035 |
0.40 |
0.40 |
0.70 |
0.60 |
N≤0.020 |
| P420NH |
≤0.20 |
≤0.50 |
1.00-
1.70 |
0.035 |
0.035 |
0.40 |
0.40 |
0.70 |
0.60 |
N≤0.020 |
| P420NL |
≤0.20 |
≤0.50 |
1.00-
1.70 |
0.030 |
0.030 |
0.40 |
0.40 |
0.70 |
0.60 |
N≤0.020 |
| P460N |
≤0.20 |
≤0.50 |
1.00-
1.70 |
0.035 |
0.035 |
0.70 |
0.40 |
1.00 |
0.70 |
N≤0.020 |
| P460NH |
≤0.20 |
≤0.50 |
1.00-
1.70 |
0.035 |
0.035 |
0.70 |
0.40 |
1.00 |
0.70 |
N≤0.020 |
| P460NL |
≤0.20 |
≤0.50 |
1.00-
1.70 |
0.030 |
0.030 |
0.70 |
0.40 |
1.00 |
0.70 |
N≤0.020 |
①表中为中厚板(厚3-70mm)的钢号及化学成分。P×××NH为磷、硫含量较高的钢;P×××NL为磷、硫含量较低的钢。
②对于厚度≤6mm的钢板,其w(Mn)含量可降低0.2%。
③每个钢号至少应添加一种细化晶粒元素,其含量范围规定如下:酸溶铝≤0.015%,w(Nb)0.015%-0.016%;w(T1)0.025%-0.20%;w(V)0.02%-0.15%。
④经供需双方商定,可调整钢中C和N含量,w(C)≤0.22%,w(N)≤0.030%。
2.ISO标准正火状态供应的细晶粒承压钢板的力学性能,见表4-2-25
表4-2-25 正火状态供应的细晶粒承压钢板的力学性能
| 钢号 |
钢板厚度/mm |
力学性能 |
热处理 |
| ≥/MPa |
ъ≥/MPa |
δ① % |
种类 |
奥氏体化温度/℃ |
冷却条件 |
|
P355N
P355NH
P355NL |
≤16
>16-35
≥35-50
>50-70 |
355
355
345
325 |
490-610 |
22 |
N(+T) |
840-940 |
空冷 |
|
P390N
P390NH
P390NL |
≤16
>16-35
≥35-50
>50-70 |
390
380
370
350 |
510-650 |
20 |
N(+T) |
840-940 |
空冷 |
|
P420N
P420NH
P420NL |
≤16
>16-35
≥35-50
>50-70 |
420
410
400
380 |
540-680 |
19 |
N(+T) |
840-940 |
空冷 |
|
P460N
P460NH
P460NL |
≤16
>16-35
≥35-50
>50-70 |
460
450
440
420 |
570-720 |
17 |
N(+T) |
840-940 |
空冷 |
①采用短试样,Lo-5.65∫SoN(+T)-正火,或正火+回火。
二、ISO标准热处理状态供应的细晶粒承压钢板[ISO26S4/8:1985]
1.ISO标准热处理状态供应的细晶粒承压钢板的钢号与化学成分,见表4-2-26
表4-2-26 热处理状态供应的细晶粒承压钢板的钢号与化学成分(质量分数)(%)
| 钢号 |
C |
Si |
Mn |
P≤ |
S≤ |
Cr≤ |
Mo≤ |
Ni≤ |
Cu≤ |
B≤ |
其他 |
| P420Q |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P420QH |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P420QL |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.025 |
0.025 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P460Q |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P460QH |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P460QL |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.025 |
0.025 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P500Q |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P500QH |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P500QL |
≤0.20 |
≤0.55 |
0.70-
1.70 |
0.025 |
0.025 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P550Q |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P550QH |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P550QL |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.025 |
0.025 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P620Q |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P620QH |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P620QL |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.025 |
0.025 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P690Q |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P90QH |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.030 |
0.030 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
| P690QL |
≤0.20 |
0.10-
0.18 |
≤1.70 |
0.025 |
0.025 |
2.00 |
1.00 |
2.00 |
1.50 |
0.005 |
N≤0.020 |
2.ISO标准热处理状态供应的细晶粒承压钢板的力学性能,见表4-2-27
表4-2-27 热处理状态供应的细晶粒承压钢板的力学性能
| 钢号 |
钢板厚度①
/mm |
屈服点
≥/MPa |
抗拉强度
/MPa |
伸长率②
≥/MPa |
|
P420Q
P420QH
P420QL |
3-50
>50-70 |
420
420 |
530-680
530-680 |
18
18 |
|
P460Q
P460QH
P460QL |
3-50
>50-70 |
460
460 |
570-720
570-720 |
17
17 |
|
P500Q
P500QH
P500QL |
3-50
>50-70 |
500
480 |
620-770
620-770 |
16
16 |
|
P550Q
P550QH
P550QL |
3-50
>50-70 |
550
530 |
670-820
670-820 |
16
16 |
|
P620Q
P620QH
P620QL |
3-50
>50-70 |
620
620 |
740-890
740-890 |
15
15 |
|
P690Q
P90QH
P690QL |
3-50
>50-70 |
690
670 |
780-930
780-930 |
14
14 |
①钢板经淬火加回火处理。
②采用短试样,Lo=5.65∫So。
三、ISO标准不同温度下使用的承压无缝钢管
2.ISO标准室温使用的承压无缝钢管的钢号与化学成分[ISO9329/1:1989],见表4-2-28。
表4-2-28 室温使用的承压无缝钢管的钢号与化学成分(质量分数)(%)
| 钢号 |
C |
Si |
Mn |
P≤ |
S≤ |
| TS360 |
≤0.17 |
≤0.35 |
0.30-0.80 |
0.040 |
0.040 |
| TS410 |
≤0.21 |
≤0.35 |
0.40-1.20 |
0.040 |
0.040 |
| TS430 |
≤0.21 |
≤0.35 |
0.40-1.20 |
0.040 |
0.040 |
| TS500 |
≤0.22 |
≤0.55 |
≤1.60 |
0.040 |
0.040 |
2.ISO标准高温使用的承压无缝钢管的钢号与化学成分[ISO 9329/2:1997],见表4-2-29。
表4-2-29 高温使用的承压无缝钢管的钢号与化学成分(质量分数)(%)
| 钢号 |
C |
Si |
Mn |
P≤ |
S≤ |
Cr |
Mo |
Ni |
其他 |
| PH23 |
≤0.17 |
0.10-
0.35 |
0.30-
0.80 |
0.035 |
0.035 |
- |
- |
- |
Cu≤0.25 |
| PH26 |
≤0.21 |
0.10-
0.35 |
0.40-
1.20 |
0.035 |
0.035 |
- |
- |
- |
Cu≤0.25 |
| PH29 |
≤0.22 |
0.10-
0.40 |
0.65-
1.50 |
0.035 |
0.035 |
- |
- |
- |
Cu≤0.25 |
| PH35 |
≤0.22 |
0.15-
0.55 |
1.00-
1.50 |
0.035 |
0.035 |
- |
- |
- |
(+Nb,Ti,V) |
| 8CrMo4-5 |
≤0.15 |
≤0.50 |
0.30-
0.60 |
0.035 |
0.035 |
0.80-
1.25 |
0.45-
0.65 |
- |
Cu≤0.25
Al≤0.020 |
| 8CrMo5-5 |
≤0.15 |
0.50-
1.00 |
0.30-
0.60 |
0.030 |
0.030 |
1.00-
1.50 |
0.45-
0.65 |
- |
Cu≤0.25
Al≤0.020 |
|
9NiMnMoNb
5-4-4 |
≤0.17 |
0.25-
0.50 |
0.80-
1.20 |
0.030 |
0.030 |
≤0.30 |
0.25-
0.40 |
1.00-
1.30 |
Nb0.015-0.045
Cu≤0.25
Al≤0.020 |
|
11CrMo
9-10TA |
0.08-
0.15 |
0.15-
0.40 |
0.30-
0.70 |
0.035 |
0.035 |
2.00-
2.50 |
0.90-
1.20 |
- |
Cu≤0.25
Al≤0.020 |
|
11CrMo
9-10TN-TT |
0.08-
0.15 |
0.15-
0.40 |
0.30-
0.70 |
0.035 |
0.035 |
2.00-
2.50 |
0.90-
1.20 |
- |
Cu≤0.25
Al≤0.020 |
| 12CrMo6-2 |
0.10-
0.15 |
0.15-
0.35 |
0.40-
0.70 |
0.035 |
0.035 |
0.30-
0.60 |
0.50-
0.70 |
- |
V0.22-0.28
Cu≤0.25
Al≤0.020 |
| 13CrMo4-5 |
0.10-
0.17 |
0.15-
0.35 |
0.40-
0.70 |
0.035 |
0.035 |
0.70-
1.10 |
0.45-
0.65 |
- |
Cu≤0.25
Al≤0.020 |
| 16Mo3 |
0.12-
0.20 |
0.15-
0.35 |
0.40-
0.80 |
0.035 |
0.035 |
- |
0.25-
0.35 |
- |
Cu≤0.25
Al≤0.020 |
|
X10CrMoVNb
9-1 |
0.08-
0.12 |
0.20-
0.50 |
0.30-
0.60 |
0.020 |
0.020 |
8.00-
9.50 |
0.85-
1.05 |
≤0.40 |
V0.18-0.25
Nb0.06-0.10
Cu0.50-0.80
Al≤0.020
N0.030-0.070 |
|
X11CrMo
5TA |
0.08-
0.15 |
0.15-
0.50 |
0.30-
0.60 |
0.030 |
0.030 |
4.00-
6.00 |
0.45-
0.65 |
- |
Cu≤0.25
Al≤0.020 |
|
X11CrMo5
TN-TT |
0.08-
0.15 |
0.15-
0.50 |
0.30-
0.60 |
0.030 |
0.030 |
4.00-
6.00 |
0.45-
0.65 |
- |
Cu≤0.25
Al≤0.020 |
|
X11CrMo
9-1TA |
0.08-
0.15 |
0.25-
1.00 |
0.30-
0.60 |
0.030 |
0.030 |
8.00-
10.00 |
0.90-
1.10 |
- |
Cu≤0.25
Al≤0.020 |
|
X11CrMo
9-1TN-TT |
0.08-
0.15 |
0.25-
1.00 |
0.30-
0.60 |
0.030 |
0.030 |
8.00-
10.00 |
0.90-
1.10 |
- |
Cu≤0.25
Al≤0.020 |
|
X12CrMoNV
11-1-1 |
0.17-
0.23 |
0.15-
0.50 |
≤1.00 |
0.030 |
0.030 |
10.0-
12.0 |
0.80-
1.20 |
0.30-
0.80 |
V0.25-0.35
Cu≤0.25
Al≤0.020 |
3.ISO标准低温使用的承压无缝钢管的钢号与化学成分[ISO 9329/3:1997],见表4-2-30。
表4-2-30 低温使用的承压无缝钢管的钢号与化学成分(质量分数)(%)
| 钢号 |
C |
Si |
Mn |
P≤ |
S≤ |
Cr |
Mo |
Ni |
其他 |
| PL21 |
≤0.17 |
≤0.35 |
0.40-
1.00 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| PL23 |
≤0.19 |
≤0.35 |
0.60-
1.20 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| PL25 |
≤0.17 |
≤0.35 |
0.40-
1.00 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| PL26P |
≤0.20 |
≤0.35 |
0.80-
1.40 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| 11MnN15-3 |
≤0.14 |
≤0.50 |
0.70-
1.50 |
0.030 |
0.025 |
- |
- |
0.30-
0.80 |
V≤0.05
Nb≤0.05
Al≤0.020① |
| 12Ni4 |
≤0.15 |
0.15-
0.35 |
0.30-
0.85 |
0.025 |
0.020 |
- |
- |
3.25-
3.75 |
V≤0.05 |
| 13MnNi6-3 |
≤0.18 |
≤0.50 |
0.85-
1.65 |
0.030 |
0.025 |
- |
- |
0.30-
0.85 |
V≤0.05
Nb≤0.05
Al≤0.020① |
| 26CrMo4 |
0.22-
0.29 |
≤0.35 |
0.50-
0.80 |
0.030 |
0.025 |
0.90-
1.20 |
0.15-
0.30 |
- |
- |
| X10Ni9 |
≤0.13 |
0.15-
0.35 |
0.30-
0.80 |
0.025 |
0.020 |
- |
≤0.10 |
8.50-
9.50 |
V≤0.05 |
| X12Ni5 |
≤0.15 |
≤0.35 |
0.30-
0.80 |
0.025 |
0.020 |
- |
- |
4.50-
5.30 |
V≤0.05 |
①系全铝含量。
四、ISO标准不同温度下使用的承压焊接钢管
1.ISO标准室温使用的承压焊接钢管的钢号与化学成分[ISO9330/1:1990]见表4-2-31
表4-2-31 室温使用的承压焊接钢管的钢号与化学成分(质量分数)(%)
| 钢号 |
C |
Si |
Mn |
P≤ |
S≤ |
| TW320 |
≤0.16 |
- |
0.30-0.70 |
0.040 |
0.040 |
| TW360 |
≤0.17 |
≤0.35 |
0.30-0.80 |
0.040 |
0.040 |
| TW410 |
≤0.21 |
≤0.35 |
0.40-1.20 |
0.040 |
0.040 |
| TW430 |
≤0.21 |
≤0.35 |
0.40-1.20 |
0.040 |
0.040 |
| TW500 |
≤0.22 |
≤0.55 |
0.40-1.20 |
0.040 |
0.040 |
2.ISO标准高温使用的承压焊接钢管的钢号与化学成分[ISO 9330/2:1997],见表4-2-32。
表4-2-32 高温使用的承压焊接钢管的钢号与化学成分(质量分数)(%)
| 钢号 |
C |
Si |
Mn |
P≤ |
S≤ |
Cr |
Mo |
其他 |
| PH23 |
≤0.17 |
≤0.35 |
0.40-1.20 |
0.035 |
0.030 |
- |
- |
- |
| PH26 |
≤0.20 |
≤0.35 |
0.50-1.40 |
0.035 |
0.030 |
- |
- |
- |
| PH27 |
≤0.20 |
≤0.35 |
0.90-1.50 |
0.035 |
0.030 |
- |
- |
- |
| PH35 |
≤0.22 |
≤0.35 |
0.90-1.60 |
0.035 |
0.030 |
- |
- |
- |
| 11CrMo9-10 |
0.08-0.15 |
0.15-0.35 |
0.30-0.70 |
0.035 |
0.030 |
2.00-2.50 |
0.90-1.10 |
Al≤0.020① |
| 13CrMo4-5 |
0.08-0.18 |
0.15-0.35 |
0.40-1.00 |
0.035 |
0.030 |
0.70-1.15 |
0.40-0.60 |
Al≤0.020① |
| 16Mo3 |
0.12-0.20 |
0.15-0.35 |
0.40-0.80 |
0.035 |
0.030 |
≤0.30 |
0.25-0.35 |
Al≤0.020① |
①系全铝含量。
3.ISO标准低温使用的承压焊接钢管的钢号与化学成分[ISO 9330/2:1997],见表4-2-33。
表4-2-33 低温使用的承压焊接钢管的钢号与化学成分(质量分数)(%)
| 钢号 |
C |
Si |
Mn |
P≤ |
S≤ |
Cr |
Mo |
Ni |
其他 |
| PL21 |
≤0.17 |
≤0.35 |
0.40-
1.00 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| PL23 |
≤0.19 |
≤0.35 |
0.60-
1.20 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| PL25 |
≤0.17 |
≤0.35 |
0.40-
1.00 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| PL26P |
≤0.20 |
≤0.35 |
0.80-
1.40 |
0.030 |
0.025 |
- |
- |
- |
Al≤0.015① |
| 11MnN15-3 |
≤0.14 |
≤0.50 |
0.70-
1.50 |
0.030 |
0.025 |
- |
- |
0.30-
0.80 |
V≤0.05
Nb≤0.05
Al≤0.020① |
| 12Ni4 |
≤0.15 |
0.15-
0.35 |
0.30-
0.85 |
0.025 |
0.020 |
- |
- |
3.25-
3.75 |
V≤0.05 |
| 13MnNi6-3 |
≤0.18 |
≤0.50 |
0.85-
1.65 |
0.030 |
0.025 |
- |
- |
0.30-
0.85 |
V≤0.05
Nb≤0.05
Al≤0.020① |
| X12Ni5 |
≤0.15 |
≤0.35 |
0.30-
0.80 |
0.025 |
0.020 |
- |
- |
4.50-
5.30 |
V≤0.05 |
①系全铝含量。 |